.064 is pretty standard for the returns on smaller boxes, nothing wrong with it. Where it starts to bite you is the bigger cabinets. The sides oil can and ripple in the sun, so most shops go up to .080 or .090 there, or keep the .064 and put an angle frame inside so the skin isn't doing all the work.
If cost is the goal, look at labor before metal. Extrusion cabinets go together fast and the faces just slide or snap in, so you're cutting and screwing instead of bending and welding every box. For small single face boxes some guys route and fold ACM into a pan. It's light and cheap, but I wouldn't do a big lit cabinet that way, it can bow when it gets hot.
Steel's cheaper per sheet but it's heavy and any cut edge that isn't primed right will rust, so outside I'd stay with aluminum.