Couple things that helped us. On solvent prints we let them gas out at least 24 hours before laminating, longer if the ink was heavy. Lam them too soon and the solvent trapped underneath softens things up, and you get exactly that shrink and curl at the edges a year or two in.
Then which way the overlap goes. On a horizontal seam put the top panel over the bottom one like shingles, so water runs off the seam instead of into it. Vertical seams don't hold water, so they usually last better. I'd go vertical when the layout lets you.
I'd also bump the overlap to about an inch, wipe the overlap with alcohol before the top panel goes on, and post heat the seam. And like unclebun said, if it's calendared it's going to shrink no matter what, so for anything outside more than a couple years go cast print vinyl with a matching cast lam.